Pure nickel and nickel alloy

N5/N6/N7/NY1

It has the following characteristics:

Nickel has high chemical stability and good corrosion resistance in many media. Its standard electrode position is -0.25v, which is positive than iron and negative than copper. Nickel has good corrosion resistance in dilute non-oxidizing properties (such as HCU, and H2SO4) and in the absence of dissolved oxygen, especially in neutral and alkaline solutions. That's because nickel has passivation ability, forming a dense protective film on the surface, which prevents the continuous oxidation of nickel.

Pure nickel and nickel alloy

Main application fields:

Chemical industry, wet corrosion-resistant parts of generator (water inlet heater and steam pipeline), pollution control equipment (waste gas desulfurization equipment), etc.

Table 1. Brand and standard


Pipes

Plates

Bar

Forging


(chemical composition)


N6

GB/T 2882-2005

GB/T 2054-2005

GB/T 4435-84

GB/T 5235-2007

NY1


GB/T 2056-2007



Table 2: chemical composition


Ni

Co

Cu

Si

Mn

C

S

Fe

Mg

P

Pb

N5


≥99.0

≤0.25

≤0.30

≤0.35

≤0.02

≤0.01

≤0.40

—

—

——

N6

≥99.5

≤0.10

≤0.10

≤0.05

≤0.10

≤0.005

≤0.10

≤0.10

0.002

≤0.002

N7

≥99.0

≤0.25

≤0.30

≤0.35

≤0.15

≤0.01

≤0.10

—

—

——

NY1

≥99.7

≤0.10

≤0.10

≤0.10

—

≤0.10

—

≤0.005

≤0.20

——

Table 3: mechanical properties of the alloy at room temperature

Name


Status

Tensile Strength
MPa

Extensibility %

Yield point

MPa

Brinell hardness

HB

Elastic limit

MPa

impact toughness


Pure nickel

annealing

294-588

10-30

≥117.6

90-120

≥78.4

≥31

cold-work

490-882

2-20

≥686

120-240

—

—